The technological process of preparing metal tungsten powder with metallurgical tungsten material includes the following steps: concentrating coarse Na2WO4 solution to crystallize and recovering excessive alkali, dissolving Na2WO4 crystal to obtain solution with WO3 concentration of 180-250 g/l and pH value of 7.5-8.5, adding alkali metal salt and evaporating to crystallize, treating the crystallized product in hydrogen atmosphere at 350-450 deg.c for 2 hr to obtain 'bluish tungsten' or calcining the crystallized product at 600-700 deg.c to obtain 'yellowish tungsten', and final reduction with hydrogen at 750-850 deg.c to obtain metal tungsten.